      "Carbonized wood" gluing properties and surface finishing, good performance, and pine in the heat treatment process, turpentine basically volatile resin has cured, therefore, the resin ducts and Setsuko surface, do not do special sealing process can be directly do finishes. Carbonized wood outdoor chairs in use, it will not happen hot weather resin overflow, destroying the paint surface problems.

      Kiln and tank "carbonized wood" outdoor chair production process are divided into primary drying and secondary drying, charring rapid heating, cooling and conditioning treatment, and then cooling the kiln (tank) 5 phase.

      1 Primary Drying

      From birth (wet) wood dried to approximately 12% (or 10%) moisture phase is called once dry. This stage can be in the kiln carbonization (tank) carried, also accomplished by conventional kiln. Given carbonization kiln (tank) of the cost is higher, and the high cost of equipment operation, so using conventional drying kiln for a more economical, and the drying quality is also easier to control, but the drying time.

      (2) second drying

      From 12% dried to a wood moisture content of 3% (or 4%) of the second drying phase is called. This phase carbonization furnace (tank) to complete. Moisture content of about 12% of the timber into the carbonization kiln, the first transition can be conventional drying. Dry bulb temperature from about 65-75 ℃ Start, and then heated in stages to about 125 ℃, wet bulb temperature gradually expanded to 25 ℃. Subject wood moisture content to about 3%, the secondary drying stage ends. This phase of the length of time, depending on the wood species and thickness, 22mm thick timber normally takes more than 10 hours.

      3 rapid heating carbonization

      Wood moisture content of 3% after, they spent the dry dangerous period. Can quickly heat up, in a relatively short period of time, rising carbonization temperature (usually 180 ~ 212 ℃). Carbonization temperature then held constant for about 3 hours, high temperature heat treatment of wood, the wood of the hemicellulose and amorphous cellulose degradation, wood moisture greatly reduce the number of hydroxyl groups. Meanwhile in wood extractives such as resin, terpenoids, tannins, acids, a large number of objects containing volatile. Thus greatly reduced hygroscopicity of wood, dimensional stability and significantly improved corrosion resistance. This stage, the kiln (tank) to be filled within a protective gas (usually water vapor), oxygen gas must be less than 2%, a simple measure of the kiln to maintain the wet-bulb temperature of 99.5 ~ 100 ℃.Otherwise, there will be very dry wood fire hazard, and the wood under high temperature oxidation, its strength is also unfavorable.

      4 cooling humidity

      Wood carbonization treatment, not only the water content is very low (0.5%), and the wood itself, the temperature is high, close to 180 ~ 212 ℃. Then the humidity can not be directly processed must first timber to cool. Note do not use air cooling, if the kiln outside in the fresh air flow into the kiln, it is easy to make wood fire. The correct way is to stop the radiator heating while spraying atomized water to the kiln, not only play a role in cooling, but also make almost all dry timber proper humidification.Subject to the kiln medium temperature dropped about 116 ℃, humidity conditioning treatment can be carried out. Then the kiln while the saturated water vapor injection, and then atomized water spray in order to enhance the relative humidity of the kiln medium moisture content of wood, and to eliminate the residual stress. Wood moisture content generally be increased from 4 to 5%, to end the humidity treatment.

      聯系我們

      聯系人:陳先生

      手機:13521257486

      電話:010-82921102

      郵箱:zhitong_chenfei@163.com

      地址: 北京市海淀區(qū)

      主站蜘蛛池模板: 色老头一区二区三区| 国产精品点击进入在线影院高清 | 在线观看视频福利| 午夜无码区在线观看| 亚洲成本人无码薄码区| 日韩在线国产| AV老司机色爱区综合| 无码av中文出轨人妻| 亚洲精品福利| 欧美在线播放一区| 亚洲精品一区二区三区色| 国产成人无码精品一区不卡| 日本大尺度做爰呻吟| 香蕉视频黄污| 又大又粗又爽18禁免费看| 国产精成人品一区| 就爱av| 久中文字幕| 18禁无遮挡啪啪无码网站| 国产高清-国产av| 91福利小视频| 午夜通通国产精品福利| 强制高潮18xxxxhd日韩| 三级在线观看| 日韩久久久精品| 精品国产中文字幕av| 嘿咻嘿咻男女免费专区| 亚洲高清视频在线观看| 北条麻妃青青久久| 欧美成人片一区二区三区| 99国产精品白浆无码流出| 国产天堂av| 能看av的网址| 少妇放荡的呻吟干柴烈火动漫| 尤物yw午夜国产精品大臿蕉| 91直接看| 精品人妻一区二区三区潮喷在线| 久久久综合九色合综| 又大又粗欧美成人网站| 久婷婷| 日本大尺度激情做爰hd|